Written by Jackson B.
Recommended slicer settings for OzFDM ASA-CF on the Bambu Lab H2D.
Nozzle Temp270 °CRange: 250 – 280 °C |
Bed Temp110 °CRange: 100 – 120 °C |
Print Speed50mm/s · max 60 |
Layer Height0.20mm · max 0.28 |
Fan Speed10 %1st layer: 0 % |
1st Layer Speed20mm/s |
Retraction0.8 mm@ 30 mm/s |
Nozzle TypeHardenedRequired |
|
Full Settings Reference
Settings |
Recommended |
Range |
Nozzle Temperature |
260 – 275 °C |
250 – 280 °C |
Bed Temperature |
100 – 110 °C |
100 – 120 °C |
Print Speed |
40 – 60 mm/s |
data sheet: 40 – 60 mm/s |
First Layer Speed |
20 mm/s |
slower is better for adhesion |
Layer Height |
0.16 – 0.24 mm |
0.12 – 0.28 mm |
Fan Speed (Normal) |
0 – 20 % |
– |
Fan Speed (1st Layer) |
0 % |
– |
Retraction Distance |
0.8 mm |
Direct drive |
Retraction Speed |
30 mm/s |
– |
Nozzle Type |
Hardened steel (required) |
0.6 mm is ideal, 0.4 mm works, never 0.2 mm |
Dry Filament |
80 °C for at least 5 h |
dry thoroughly before every long print |
Enclosure |
Required, door closed |
chamber heating off for small parts, 60 °C for large parts (H2D maximum 65 °C) |
Support Material |
HIPS, ASA-CF (interface) |
– |
|
|
Printing Notes |
|
|
ASA-CF is abrasive, so print it only through a hardened steel nozzle. The H2D's stock 0.4 mm nozzles are hardened steel, but check any hotend you have swapped in. |
|
|
OzFDM suggests a 0.6 mm hardened steel nozzle as the ideal size for ASA-CF, since a larger nozzle is less prone to fibre clogs. The figures above are for 0.4 mm. Do not use a 0.2 mm nozzle. |
|
|
Our ASA-CF product page and Bambu Lab both advise against running third-party carbon fibre filament through the AMS, so feed it from an external spool holder or a sealed dry box. Parts are stiffer but more brittle than plain ASA, so handle spools and prints with care. |
|
|
ASA-CF gives off fumes while printing. Keep the door closed, print in a ventilated room and use air filtration. For large parts, set the chamber to about 60 °C in the Bambu Studio filament settings. |
|
|
Slicer: Bambu Studio. Start from the Generic ASA filament preset and set the temperatures above. Every figure assumes dry filament, so dry at 80 °C for at least 5 h before a long print. |
Tested on our Bambu Lab H2D with a 0.4 mm hardened steel nozzle, September 2026.
|
Troubleshooting |
|
Intermittent under-extrusion or a partial clog: Fibre is packing in the nozzle. Dry the filament, clear the nozzle with a cold pull, and consider a 0.6 mm hardened steel nozzle. |
|
Filament snaps in the feed path: ASA-CF is more brittle than plain ASA. Dry it and avoid tight bends in the PTFE tube. |
|
Warping on long parts: Keep the bed at 110 °C, turn on chamber heating at 60 °C, add a brim and let the chamber warm up before the first layer. |
OzFDM ASA-CF Filament
-
Carbon fibre reinforced ASA with a matte finish, high stiffness and low warping for outdoor functional parts.