Written by Jackson B.
Recommended slicer settings for OzFDM PETG Basic on the Bambu Lab H2D.
Nozzle Temp235 °CRange: 220 – 240 °C |
Bed Temp70 °CRange: 70 – 80 °C |
Print Speed80mm/s · max 120 |
Layer Height0.20mm · max 0.28 |
Fan Speed40 %1st layer: 0 % |
1st Layer Speed20mm/s |
Retraction0.8 mm@ 30 mm/s |
Nozzle TypeHardenedStock 0.4 mm |
|
Full Settings Reference
Settings |
Recommended |
Range |
Nozzle Temperature |
230 – 240 °C |
220 – 240 °C |
Bed Temperature |
70 – 80 °C |
70 – 80 °C |
Print Speed |
60 – 120 mm/s |
data sheet: 40 – 250 mm/s |
First Layer Speed |
20 mm/s |
slower is better for adhesion |
Layer Height |
0.16 – 0.24 mm |
0.12 – 0.28 mm |
Fan Speed (Normal) |
30 – 50 % |
– |
Fan Speed (1st Layer) |
0 % |
– |
Retraction Distance |
0.8 mm |
Direct drive, up to 1.2 mm |
Retraction Speed |
30 mm/s |
– |
Nozzle Type |
Hardened steel (stock) |
any 0.4 mm nozzle suits this material |
Dry Filament |
70 °C for 5 h |
store sealed with desiccant between prints |
Enclosure |
Not required, chamber heating off |
a hot chamber can soften PETG in the extruder |
Support Material |
PVA, PLA (interface) |
– |
|
|
Printing Notes |
|
|
PETG Basic comes on a slimmer spool that some AMS units do not recognise during automatic loading. Move it onto an AMS-compatible reusable spool, or feed it from the external spool holder. |
|
|
PETG bonds very strongly to smooth PEI. Print on the Textured PEI Plate, or use a thin layer of glue stick as a release layer on smooth PEI. |
|
|
Leave chamber heating off. Bambu Lab groups PETG with the low-temperature filaments that can soften and clog in a hot chamber, so let the H2D run PETG with its chamber vented. |
|
|
Bambu Lab's filament guide lists 240 – 270 °C for PETG, above OzFDM PETG Basic's 220 – 240 °C range, so change the nozzle temperature before slicing. A heat deflection temperature of 74 °C suits parts that sit somewhere warm. |
|
|
Slicer: Bambu Studio. Start from the Generic PETG filament preset and set the temperatures above. Every figure assumes dry filament, so dry at 70 °C for 5 h before a long print. |
Tested on our Bambu Lab H2D with a 0.4 mm nozzle, September 2026.
|
Troubleshooting |
|
Stringing and blobs: Dry the roll at 70 °C for 5 h first, then drop the nozzle to 230 °C. Tune retraction last. |
|
First layer too squashed or rough: Slow the first layer to 15 mm/s and check the plate type selected in Bambu Studio matches the plate fitted, since bed temperature is set per plate type. |
|
Parts split between layers under load: Cooling is too high. Drop the fan to 30 % and raise the nozzle 5 °C, staying at or below 240 °C. |
OzFDM PETG Basic Filament
-
Tough, glossy everyday PETG for brackets, enclosures and functional parts.