PLA on Voron Trident

PLA on Voron Trident - OzFDM

Recommended slicer settings for OzFDM PLA Basic on the Voron Trident.

Nozzle Temp

210 °C

Range: 190 – 230 °C

Bed Temp

55 °C

Range: 25 – 60 °C

Print Speed

70

mm/s · max 120

Layer Height

0.20

mm · max 0.32

Fan Speed

100 %

1st layer: 20 %

1st Layer Speed

25

mm/s

Retraction

0.6 mm

@ 45 mm/s

Nozzle Type

Brass

Standard


Retraction Note

  • Klipper's pressure advance handles most ooze. Short retraction with fast CoreXY.


Full Settings Reference

Settings

Recommended

Range

Nozzle Temperature

200 – 215 °C

190 – 230 °C

Bed Temperature

50 – 60 °C

25 – 60 °C

Print Speed

60 – 90 mm/s

up to 120 mm/s on this printer

First Layer Speed

20 – 35 mm/s

slower is better for adhesion

Layer Height

0.16 – 0.24 mm

0.08 – 0.32 mm

Fan Speed (Normal)

100 %

Fan Speed (1st Layer)

0 – 30 %

Retraction Distance

0.6 mm

Direct drive

Retraction Speed

45 mm/s

Nozzle Type

Brass (standard)

Brass is fine; hardened optional

Dry Filament

40 – 45 °C for 4 – 6 h

print from a dry box in humid weather

Enclosure

Not required

Not required — helps in a cold or draughty room

Support Material

PVA, PETG (interface)

Printing Notes

PLA Basic shares its print window with OzFDM PLA+ but is a little stiffer and more brittle, so it suits display pieces and prototypes rather than parts that flex.

It is the cheapest way to dial in a new printer — run your first-layer and flow calibration on PLA Basic before moving to anything expensive.

Klipper's pressure advance does most of the ooze control on a Trident, so short fast retraction beats long slow retraction here.

As a self-built machine the Trident's chamber temperature is whatever you have built it to hold — check it before starting a high-temperature print rather than assuming.

Slicer: OrcaSlicer / SuperSlicer (Klipper). Dry the filament at 40 – 45 °C / 4 – 6 h before a long print — every figure above assumes dry filament.

Troubleshooting

Brittle parts that snap along layer lines — Raise the nozzle 5 °C and drop cooling to 80 % on tall thin parts. PLA Basic is less forgiving of over-cooling than PLA+.

Stringing — Dry the roll and drop to 200 °C. Stringing in PLA is almost always heat or moisture, not retraction.

Poor first layer — PLA Basic likes a 60 °C bed even though it will stick at 25 °C. Warm the bed properly and slow the first layer.

OzFDM PLA Basic Filament