ASA on Bambu Lab X1 Carbon

ASA on Bambu Lab X1 Carbon - OzFDM

Recommended slicer settings for OzFDM ASA on the Bambu Lab X1 Carbon.

 

 Nozzle Temp

250 °C

Range: 240 – 260 °C

Bed Temp

110 °C

Range: 100 – 120 °C

Print Speed

50

mm/s · max 60

Layer Height

0.20

mm · max 0.28

Fan Speed

10 %

1st layer: 0 %

1st Layer Speed

20

mm/s

Retraction

0.9 mm

@ 30 mm/s

Nozzle Type

Brass

Standard


 

  Retraction Note

  • Keep retraction minimal like ABS. ASA is more prone to stringing than ABS but less than PETG.


Full Settings Reference

 Settings

Recommended

Range

Nozzle Temperature

250 °C

240 – 260 °C

Bed Temperature

110 °C

100 – 120 °C

Print Speed

40 – 60 mm/s

up to 60 mm/s on this printer

First Layer Speed

20 mm/s

slower is better for adhesion

Layer Height

0.16 – 0.24 mm

0.12 – 0.28 mm

Fan Speed (Normal)

0 – 20 %

Fan Speed (1st Layer)

0 %

Retraction Distance

0.9 mm

Direct drive

Retraction Speed

30 mm/s

Nozzle Type

Brass (standard)

Brass is fine; hardened optional

Dry Filament

80 °C for ≥ 5 h

print from a dry box in humid weather

Enclosure

Required, built in

Required, this printer is enclosed

Support Material

HIPS, ASA (self-supporting)

 

 

 Printing Notes

 

ASA is the outdoor material. It holds colour and impact strength under Australian UV where ABS chalks and yellows within a season.

 

It is more impact-resistant than ABS, 19 – 20 kJ/m² against 7 – 10.5, and warps slightly less, but it still needs an enclosure.

 

The X1C ships with a hardened steel nozzle and a fully enclosed chamber, so it needs none of the modifications other machines do for this material.

 

Bambu Studio's own generic profile is a reasonable starting point, but its temperatures are set for Bambu filament, so use the figures above for OzFDM spools.

 

Slicer: Bambu Studio / OrcaSlicer. Dry the filament at 80 °C / ≥ 5 h before a long print. Every figure above assumes dry filament.

 

 Troubleshooting

 

Warping despite an enclosure. ASA runs hotter than ABS. Take the bed to the top of what your machine allows and let the chamber come up to temperature before the print starts, not during it.

 

Weak layer bonding. Cooling is on. ASA wants the fan off entirely except for bridges.

 

Surface blistering or bubbling. Damp filament. Dry at 80 °C for at least five hours. ASA's listed moisture absorption is 0.35 % at 23 °C and 50 % relative humidity, at equilibrium.

 

OzFDM ASA Filament