Thread-Forming Screws vs Heat-Set Inserts vs Nut Traps: Which Joint to Use

SS304 thread-forming screws for plastics with countersunk and pan washer heads

Written by Logan F.

Quick answer: Use thread-forming screws for parts you assemble once or rarely, heat-set inserts for joints you open often or tighten firmly, and nut traps where you want the most pull-out strength with only a hex key. In CNC Kitchen's M3 tests, inserts took about three times the torque of a screw driven straight into plastic.

Printed parts need threads, and plastic makes a poor thread on its own. There are three practical ways to get a solid screw joint in a print: let a thread-forming screw make its own thread, melt a brass heat-set insert into a hole, or trap a steel nut in a pocket. Each one suits a different job. This guide compares them using published test results and the specifications of the hardware we sell, then gives the design rules for each.

The three joints at a glance

Joint Tools needed Repeated assembly Strength notes Best for
Thread-forming screw Hex key Limited: the thread is plastic No extra parts; strength depends on the plastic and boss design Prototypes, covers and parts assembled once or twice
Heat-set insert Soldering iron, ideally with an insert tip Good: brass thread Highest torque in CNC Kitchen's M3 tests Lids, access panels, enclosures, parts serviced often
Nut trap Hex key, sometimes a pause mid-print Good: steel thread Highest pull-out in CNC Kitchen's PETG test when the nut sits on the far face Through-bolted joints and brackets that carry load

What the published tests show

CNC Kitchen has run two useful M3 tests. In Threaded Inserts for 3D Prints: Cheap vs Expensive, samples were printed in PLA at 100% infill. In Helicoils vs Threaded Inserts vs Embedded Nuts, samples were PETG with four perimeters and 100% infill.

M3 joint Material Pull-out (average) Maximum torque
Screw driven into a 2.7 mm printed hole PLA 142 kg About 1 Nm
Good-quality heat-set insert PLA 157–181 kg 3–4 Nm (bolt heads sheared)
Screw driven into a slightly undersized hole PETG 118 kg 1 Nm
Heat-set insert PETG 119 kg 3 Nm
Nut in a side pocket PETG 86 kg 2 Nm
Nut in a bottom pocket PETG 166 kg 2 Nm

Three things stand out. Pull-out strength for a screw straight into plastic was in the same range as a heat-set insert: 118 kg against 119 kg in PETG, and 142 kg against 157–181 kg in PLA. Torque is where inserts pulled ahead, holding about three times as much before failing. And a nut on the far face spread the load over the most plastic, giving the best pull-out result in the PETG test. CNC Kitchen also points out that even 1 Nm on an M3 bolt produces more than 1,500 N of clamping force, so a low torque limit is not necessarily a weak joint.

One caveat: those tests used standard M3 machine screws in plain holes, not screws with a thread-forming profile. Treat them as a guide to screwing directly into plastic rather than a direct test of thread-forming screws.

Thread-forming screws

A thread-forming screw is a type of self-tapping screw that displaces material to form its thread rather than cutting it away, which suits plastics. Our SS304 thread-forming screws come in 3 × 8, 3 × 15, 4 × 10 and 4 × 15 mm, with countersunk or pan washer heads and a hex drive.

Hole sizes

Screw Blind hole diameter Blind hole depth
3 × 8 mm About 1.8 mm About 12 mm
3 × 15 mm About 1.8 mm About 22 mm
4 × 10 mm About 2.5 mm About 15 mm
4 × 15 mm About 2.5 mm About 22 mm

These are the starting sizes from our product page. For pan washer head screws, add a small chamfer at the top of the hole for an easier start and room for displaced plastic. The blind holes are deeper than the screws, which leaves space below the tip.

Boss design

EJOT, the manufacturer of PT screws for plastics, publishes boss guidelines for moulded parts: a hole of about 0.7–0.8 times the screw diameter depending on the plastic, a boss outside diameter of about 1.8–2 times the screw diameter, and about 1.7–2 times the diameter of thread engagement. For a 3 mm screw, that means a boss about 6 mm across with about 6 mm of engagement. Those figures are for injection moulding, so use them as starting points for printed bosses and test.

  • If the screw is very tight or the boss splits, open the hole in 0.1–0.2 mm steps. EJOT's moulded-part holes are larger than our 1.8 and 2.5 mm starting sizes, so there is room to go up.
  • Give the thread solid plastic. Add enough walls that the whole thread sits in perimeters rather than infill. CNC Kitchen's PETG samples used four perimeters.
  • Print the boss upright where you can. A thread-forming screw pushes outwards on the hole wall. With the hole axis vertical that force acts within each layer. With the axis horizontal it pulls layers apart, and layer bonds are the weakest direction in a print, as covered in our DFM basics guide.

Refitting thread-forming screws

When you refit a screw, turn it backwards gently until you feel it drop into the existing thread, then drive it forwards. That follows the thread already formed instead of starting a new one. Stop as soon as the head seats. Our product page puts it simply: thread-forming screws suit parts you won't take apart often, and heat-set inserts give a stronger, reusable metal thread for joints you open regularly.

Heat-set inserts

A heat-set insert is a knurled brass sleeve with a metric thread inside. You heat it with a soldering iron and press it into a slightly undersized hole, the plastic flows into the knurling, and you are left with a machine thread you can tighten and undo many times. Our heat-set insert guide covers installation in detail. The key design numbers from our size chart are:

  • Hole diameters: 3.1 mm (M2 Long), 4 mm (M2.5 Long, M3 Short and M3 Long), 4.4 mm (M3 Thick), 5.5 mm (M4), 6.2 mm (M5), 7.1 mm (M6), 9.1 mm (M8) and 7.3 mm (1/4 Long).
  • Make blind holes about 1 mm deeper than the insert, as CNC Kitchen recommends.
  • Set the iron to the filament's printing temperature plus about 10°C, and press straight and slowly.

Inserts take more time per joint and need an iron, but they give you the torque advantage from the tests above, and the thread does not wear each time you open the part.

Nut traps

A nut trap holds a standard steel nut in a hex or square pocket. The thread is steel, so it lasts, and nuts are cheap and easy to replace. Sizing comes from the nut's across-flats dimension. Our guide to designing prints for metric screws and nuts has the full M2 to M8 table, clearance holes and CAD tips.

  • Put the nut on the far face of the part where you can. That is the layout that gave 166 kg of pull-out in the PETG test.
  • Use side slots when the far face is not reachable, and expect roughly half the pull-out strength.
  • Choose nyloc nuts where vibration could loosen the joint, and a washer where a nut or screw head bears on plastic.
  • For a nut fully enclosed in the part, pause the print and drop it in, as described in our guide to embedding magnets in 3D prints.

Which joint for which job

  • Quick prototype or cover you will fit once: thread-forming screw.
  • Battery door, lid or access panel opened regularly: heat-set insert.
  • Bracket or mount carrying a pulling load: through bolt with a nut on the far face.
  • Nut can only go in from the side: side slot with a hex nut, or a square nut.
  • Not sure yet: design the boss big enough for an insert. You can start with a thread-forming screw, then drill the hole out to the insert size later if the joint needs it.

Shop the materials in this guide

Frequently asked questions

Are thread-forming screws the same as self-tapping screws?

They are one kind of self-tapping screw. Thread-forming screws push material aside to form the thread, while thread-cutting screws have cutting edges that remove material. Forming suits plastics.

What pilot hole do I need for a 3 mm thread-forming screw?

Our product page recommends starting at about 1.8 mm, with a blind hole about 12 mm deep for the 3 × 8 mm screw and 22 mm deep for the 3 × 15 mm screw.

How many times can I reuse a thread-forming screw hole?

There is no fixed number. Every refit wears the plastic thread a little, so use thread-forming screws for parts you rarely open, and refit carefully by finding the existing thread first.

Are heat-set inserts always stronger than screwing into plastic?

Not in pull-out. CNC Kitchen measured pull-out in the same range for both in PLA and PETG. Inserts were clearly better in torque and give a metal thread that survives repeated assembly.